From China Lens Ring Joint Gasket manufacturer Kaxite professional supplying Lens Ring Joint Gasket. If you need Lens Ring Joint Gasket, please feel free to contact us!
From China Double Jacket Gasket manufacturer Kaxite professional supplying Double Jacket Gasket. If you need Double Jacket Gasket, please feel free to contact us!
From China Corrugated Gaskets manufacturer Kaxite professional supplying Corrugated Gaskets. If you need Corrugated Gaskets, please feel free to contact us!
From China PTFE Envelope Gasket manufacturer Kaxite professional supplying PTFE Envelope Gasket. If you need PTFE Envelope Gasket, please feel free to contact us!
From China Rubber Sheet manufacturer Kaxite professional supplying Rubber Sheet. If you need Rubber Sheet, please feel free to contact us!
Made of asbestos Fibre, rubber and heat-resisting packing material, compressing it to thick paper .
4600 x 1500 x (0.3 - 6.0)mm,4100 x 1500 x (0.3 - 6.0)mm
3800 x 2700 x (0.3 - 6.0)mm,2000 x 1500 x (0.5 - 6.0)mm
1500 x 1360 x (0.5 - 6.0)mm,3810 x 1270 x (0.5 - 6.0)mm
1270 x 1270 x (0.5 - 6.0)mm,1500 x 1500 x (0.5 - 6.0)mm
The other size is optional or according to the requirements of customers.
Packing: in wooden pallet of about 1000 kgs, 2000kgs net each.
Asbestos Rubber Sheets Physical Property
GB/T 3985-2008 |
||||||||
Item
|
KXB510
|
KXB450
|
KXB400
|
KXB350
|
KXB300
|
KXB250
|
KXB200
|
KXB150
|
Tensile strength MPa
|
21.0
|
18.0
|
15.0
|
12.0
|
9.0
|
8.0
|
6.0
|
5.0
|
Aging Coefficient
|
0.9
|
|||||||
Burning Loss %
|
28.0
|
30.0
|
||||||
Compressibility rate%
|
7-17
|
|||||||
Rebound Rate%
|
45
|
40
|
35
|
|||||
Creep relaxation rate%
|
50
|
|||||||
Density g/cm3
|
1.6 - 2.0
|
|||||||
Nitrogen leakage rate
[ml/(h.mm)] |
500
|
|||||||
Heat and pressure resistance
|
with the temperature of 500-510 and the pressure of 13-14MPa,Keep for 30 min without puncture
|
with the temperature of 440-450 and the pressure of 11-12MPa,Keep for 30 min without puncture
|
with the temperature of 390-400 and the pressure of
8-9 MPa,Keep for 30 min without puncture |
with the temperature of 340-350 and the pressure of
7-8 Mpa,Keep for 30 min without puncture |
with the temperature of 290-300 and the pressure of
4-5 MPa,Keep for 30 min without puncture |
with the temperature of 240-250 and the pressure of
3-4Mpa,Keep for 30 min without puncture |
with the temperature of 190-200 and the pressure of
2-3MPa,Keep for 30 min without |
with the temperature of 140-150 and the pressure of 1.5-2MPa,Keep for 30 min without puncture
|